JLÄñ¶½¤¡@¤Þ¶i·N¤j§QDOLCI¤½¥q³]³Æ¡A¿ï¥ÎDOW¡BEXXONµ¥¤½¥q¶i¤f½u©Ê§C±K«×»E¤A²m¡]LLDPE¡^¡A±Ä¥Î¤T¼h¦@À½¬y©µ¤uÃÀ¨î¦¨¡C¤j½¤¼e2100mm¡A°ª½¤³t500m/min¡A½¤«p15μm-50μm¡A¥i¦b½u¤À¤Á¦UºØ³W®æ¡C «öÖߩʤÀ³æ±Öß¡BÂù±Öß¡C«ö¥Î³~¤À¤â¤uÄñ¶½¤©M¾÷¥ÎÄñ¶½¤¨â¤j«Y¦C¡C
¶µ¥Ø
Properties
|
³æ¦ì
Unit
|
´ú¸Õ¤èªk
Tost Method
|
¾÷¥Î½¤
Machine Wrap Film
|
¤â¤u½¤
Hand Wrap Film
|
¤ñ«
Spectific gravity
|
g/cm3
|
ASTMD 1505
|
0.197
|
0.197
|
©Ô¦ù±j«×MD
Tensite strength at break TD
|
Kg/cm2
|
ASTMD 885
|
≥380
≥250
|
≥300
≥200
|
Â_µõ¦ùµõªø²vMD
Elongation at break TD
|
%
|
ASTMD882
|
≥400
≥700
|
≥350
≥600
|
ª½¸Ñ¼¹µõ±j«×MD
Rightangle tear strength TD
|
N/mm
|
HT
|
≥75
≤90
|
≥75
≥90
|
Öß©Ê
Adhesion
|
N/cm2
|
HT
|
≥0.8
|
≥0.8
|
Ãú«×
Haze
|
%
|
ASTMD1003
|
≤2
|
≤2
|