¾T¦Xª÷2017ªº¦¨¥÷¡B©Ê¯à»P¨å«¬¥Î³~2017ªº¦Xª÷¤¸¯À¬°»É¡A¬O²Ä¤@ÓÀò±o¤u·~À³¥Îªº2«Y¦Xª÷¡A¨ã¦³«Ü°ªªº±j«×©M¨}¦nªº¤Á«d¥[¤u©Ê¯à¡A¦ý@»G»k©Ê¸û®t¡C¥DnÀ³¥Î©ó¹g°v¡B³q¥Î¾÷±ñ¹s¥ó¡B¸¾÷¡B²î²í¡B¥æ³q¡B«Ø¿vµ²ºc¥ó¡B¹B¿é¤u¨ãµ²ºc¥ó¡BÁ³±Û¼Õ¤¸¥ó¤Î°t¥ó¡C | |||||||||
¤Æ¾Ç¦¨¤À¡]Chemical Composition Limits wt%) | |||||||||
Cu | Si | Fe | Mn | Mg | Zn | Cr | Ti | Pb.Bi | Al |
3.5-4.5 | 0.2-0.8 | 0.7 | 0.4-1.0 | 0.4-0.8 | 0.25 | 0.10 | 0.15 | / | ¾l¶q |
¨å«¬¦Xª÷2017-451¾÷±ñ©Mª«²z©Ê¯à¡]Typical Mechanical & Physical Properties) | |||||||||
²k±µ©Ê | ¤Á«d©Ê | @»k©Ê | ¹q¾É²v20°C(68°F)(%IACS¡^ | ±K«×(20°C)(g/cm3) | |||||
¸û¦n | «Ü¦n | ®t | 30-40 | 2.79 | |||||
§Ü©Ô±j«×(25°C Mpa) | ©}ªA±j«×(25°C Mpa) | µw«×500kg¤O10mm²y | ©µ¦ù²v1.6mm(1/16in)«p«× | ¤j°ÅÀ³¤OMpa | |||||
425 | 275 | 105 | 20 | 260 |